# Me Ya Sa Bussing (Overlap Soldering) Ke Haifar da Tsagewar Ƙwayoyin Rana

> Hanyoyi uku da haɗin bussing ke fashe tantanin halitta yayin lamination: rata da aka tanada wadda ta yi ƙanƙanta, ribbon da aka yi a kan mataki, da zoben solder.

![Me Ya Sa Bussing (Overlap Soldering) Ke Haifar da Tsagewar Ƙwayoyin Rana](https://cdn.ooitech.com/static/upload/image/20261016/2026101628282828.webp)

- ** Jerry
- ** 2026-07-20
- ** 374 Kallo
- ** [Blog](./Blog.html)

## Me Ya Sa Bussing (Overlap Soldering) Ke Haifar da Tsagewar Ƙwayoyin Rana

**Amsa mai sauri:** Fashewar rami na tsakiya da ke fitowa daga matakin bussing gazawa ce ta inji a haɗin tsakanin gefen tantanin da busbar. Abubuwa uku ne ke haddasa ta. Rata da aka tanada tsakanin tantanin da busbar ta yi ƙanƙanta, don haka ribbon ɗin ke ratsawa a kusurwa mai tsauri kuma yana matse gefen. An yi ribbon ɗin a kan bambancin tsayi wanda lamination daga baya ke daidaitawa, yana barin rarar ribbon wanda dole ya lanƙwasa a wani wuri. Ko kuma murfin ribbon ɗin ya narke ya zama zoben solder mai tasowa wanda ake matsewa cikin wafer. Duk ukun suna lodin gefen wafer mai kauri kusan 0.13 mm, kuma duk ukun yawanci suna bayyana ne kawai bayan lamination, a cikin electroluminescence.

Tsagewar rami na tsakiya na daga cikin mafi yawan lahani na kwalliya da layin samar da module ke haifarwa, kuma jerin abubuwan da za su iya haddasawa suna da yawa. Lalacewar jiyya, gilashi, encapsulant, kurakuran stringer da sigogin lamination duk suna da nasu alamomin. Wannan shafi ya takaita batun zuwa bangaren da ya fito daga bussing — matakin soldering na haɗuwa wanda ke haɗa ƙarshen string a kan busbar — kuma ya yi bayani kan hanyoyi uku da wannan mataki ke karya sel.

Abin da waɗannan ukun suka haɗa shi ne cewa babu ɗayansu da ya zama gazawar lantarki. Matsalolin geometry ne. Haɗin da ke tsakanin gefen sel da busbar wuri ne da wafer siriri, tsiri mai kauri da yawa na ribbon da haɗin solder suka haɗu, kuma inda tsiri da ke ƙarƙashin tashin hankali ke canza alkibla. Idan ka yi kuskuren wannan geometry da 'yan goma na millimita, wafer zai biya shi daga baya, a cikin matsi.

A ƙasa akwai tsarin kowane ɗaya daga cikin abubuwan haddasawa uku, abin da ke bambanta su da juna a kan layin, da abin da ya cancanci a auna kafin lamination maimakon bayan.

## Haɗin da wannan shafi ya kunsa

Bussing shine inda ake manna ƙarshen igiyar da aka gama a kan busbar da ke tattara wutar lantarki kuma ta kai ta zuwa akwatin haɗin wuta. A kan igiyar TOPCon, ribbon ɗin yana barin gaban tantanin halitta kuma ana manna shi a bayan busbar, don haka haɗin yana tsaye a gefen tantanin halitta maimakon a tsakiyar saman tantanin halitta.

Na'urar tana kawo tantanin halitta da busbar zuwa wani mataki ɗaya yayin aikin. Wannan ba ya sa su zama kauri ɗaya, kuma bambancin ba ƙarami ba ne:

| Abu | Kaurin da aka saba |
| --- | --- |
| Wafer na TOPCon | 0.13 mm |
| Ribbon na tsakiyar busbar | 0.35 mm zuwa 0.40 mm |

Don haka ribbon ɗin yana barin wafer na 0.13 mm, ya ketare rata, ya sauka a kan wani ɗigon da ya ninka kaurinsa kusan sau uku. Ribbon ɗin ne kaɗai memba da ke ratsa wannan matakin, kuma yana yin haka cikin tashin hankali. Inda ya taɓa gefen tantanin halitta, yana turawa. Wannan shine duk yanayin gazawar a cikin jumla ɗaya; dalilai uku da ke ƙasa su ne kawai hanyoyi uku na ƙara turawa.

## Dalili na ɗaya: ratar da aka tanada tsakanin gefen tantanin halitta da busbar ta yi ƙanƙanta

Tazarar da ke tsakanin gefen tantanin halitta da busbar wani yanki ne na tsari, ba ma'aunin ƙayyadadden girma ba. Abubuwa da yawa na yau da kullum suna tura gefen tantanin halitta kusa da busbar fiye da yadda ya kamata. Matsalolin hangen nesa na CCD a kan injin busbar na iya yin hakan. Haka kuma kuskuren matsayi a kan wannan injin na iya yin hakan. Igiyar da tsawonta gaba ɗaya ya fita daga ma'auni kuma tana yin hakan, saboda tantanin halitta na ƙarshe yakan isa wani wuri dabam da inda na'urar ke tsammani.

Da zarar tazarar ta yi guntu, ribbon ɗin dole ne ya yi irin wannan hawan a kan ɗan gajeren tafiya, don haka kusurwar da ke tsakanin ribbon ɗin da gefen wafer ɗin takan ƙara tsananta. Ɗauki ƙarfin ribbon ɗin a matsayin kusan akai-akai sannan ka raba shi zuwa sassa biyu a wurin da ribbon ɗin ya bar tantanin halitta:

- **F1** yana aiki a cikin jirgin wafer ɗin, yana jan ribbon ɗin zuwa ga busbar.
- **F2** yana aiki daidai da wafer ɗin, yana danna ribbon ɗin ƙasa a kan gefen tantanin halitta.

Tsallakewa mai zurfi yana motsa tashin hankali daga F1 zuwa F2. Jan hankali a kwance yana raguwa, matsin ƙasa yana ƙaruwa, kuma gefen shine inda wannan matsin ya isa. Silicon yana da karyewa, wafer ɗin yana da siriri, kuma gefen wani fili ne mai 'yanci ba tare da wani abu a kusa da shi don yada nauyin ba. Tsagewa yana farawa daga gefen kuma yana gudu zuwa ciki. A kan ingantaccen module yana bayyana a matsayin layi mai duhu ko faci mai duhu a cikin EL.

Wannan sanadin shine mafi sauƙi daga cikin ukun don hanawa kuma mafi wuya a gani, saboda haɗin da ya yi nesa da 0.2 mm yana kama da daidai. Kulawa ita ce jeri da kanta: daidaita hangen nesa, iyawar maimaita jeri na kan bussing, da haƙurin tsayin igiyar da ke zuwa daga [stringer](https://www.ooitech.com/tabber-and-stringer-machine-how-it-works-how-to-choose.html).

## Sanadi na biyu: an yi ribbon ɗin a kan matakin da lamination ke cirewa

Sanadi na biyu yana farawa haka, tare da bambancin tsayi tsakanin tantanin halitta da busbar a tashar bussing, amma sakamakon ya bambanta. A nan bambancin ya yi girma sosai har ribbon ɗin, da zarar an sayar da shi, yana riƙe da mataki a cikin siffarsa. An yi haɗin, an gyara ribbon ɗin, kuma tsayin ribbon ɗin a cikin wannan haɗin yanzu adadi ne da ba ya canzawa.

Lamination sannan yana yin abin da lamination yake yi: yana matse haɗin ƙasa. Filayen biyu suna zuwa daidai, kuma hanyar da ribbon ɗin zai ratsa tsakanin su tana yin guntu. Ribbon ɗin, duk da haka, ya riga ya kai tsawon da yake da shi, kuma ba zai iya guntuwa. Ragin dole ya tafi wani wuri, don haka ribbon ɗin yana lanƙwasa — kuma lanƙwasawar tana kan gefen tantanin.

Sakamakon shine lahani ɗaya da sanadi na ɗaya, tare da wata alama daban: yakan bayyana a rukuni maimakon tantanin da ya keɓe, domin matakin mallakar saitin ne ba na haɗin gwiwa ɗaya ba. Hakanan shine dalilin da yasa haɗin gwiwa zai iya wuce dubawa a tashar bussing kuma har yanzu ya haifar da tsagewa a matsi. Daidaiton saman a bussing shine wurin sarrafawa, ba kamannin haɗin gwiwa ba.

## Sanadi na uku: murfin ya narke ya zama zobe mai ɗagawa

Sanadi na uku shine mafi ƙarancin, shine mafi koyarwa, kuma shine kaɗai wanda ke farawa a matsayin shawarar siye. Ya bayyana a cikin lamarin tushe a matsayin layi mai tsayin daka na tsagewar tsakiyar rami bayan lamination. Masu lamination da yawa suna samar da lahani ɗaya kuma injin bussing shine abu ɗaya da aka gyara a hoton, wanda shine abin da ya nuna binciken zuwa matakin bussing.

Abin da ke faruwa a can: tantanin da busbar ɗin suna da ɗan bambancin tsayi, kuma a yankin cokali mai yatsu, inda busbar ɗin ya rabu zuwa ga jagororin, babu busbar a ƙarƙashin ribbon ɗin da za a yi walda da shi. Ribbon ɗin ya rabu da wafer ɗin. Zafin narkewar gami da ya narke murfin ribbon ɗin, wanda ya ja kansa ya zama ƙulli a kewayen ribbon ɗin kuma ya daskare a matsayin zobe mai ɗagawa. A ƙarƙashin matsin lamination wannan zoben ya yi aiki a matsayin wuri mai tauri a saman wafer mai rauni, kuma ya fashe shi.

Dalilin da zoben suka bayyana a rukuni shi ne abin da ya cancanci tunawa. Layin ya koma amfani da ribbon mai arha mai yawan tin da ƙarancin jan ƙarfe, kuma murfin wannan ribbon ɗin yana da bambancin kauri tare da nadi. Ƙarin solder a haɗin ya haifar da babban zobe. Komawa zuwa daidaitaccen ribbon ya kawar da lahani gaba ɗaya.

Abubuwa biyu sun biyo daga wannan. Kaurin murfi da daidaitonsa ya kamata su kasance cikin binciken shigowa maimakon a kan takardar bayanai kawai. [murfin shi ne ɓangaren ribbon ɗin da ke yin haɗin](https://www.ooitech.com/pv-ribbon-materials-copper-core-hardness-and-coating.html), kuma nada mai rufi mara daidaito yana aiki daban da mai daidaito, ko da dukansu sun cika ma'auni ɗaya. Kuma haɗin yana buƙatar wani abu a bayansa. Inda ribbon ɗin ya ratsa wani yanki da babu goyan baya, duka saida da lamination suna aiki da juzu'i maimakon da shi.

## Bambance tsakanin ukun

A kan layin da ke samar da tsagewar rami na tsakiya, yanayin lahani sau da yawa ya isa ya nuna sanadin kafin a yi wani ma'auni. Ukun da ke ƙasa su ne alamomin da suka shafi bussing; akwai wasu alamomi kuma suna nuni zuwa wani wuri.

| Abin da kuke gani | Sanadin da ake tsammani | Abu na farko da za a duba |
| --- | --- | --- |
| Tsagewa da ke bin hanyar busbar, suna bayyana a kan sel waɗanda duk haɗin su ya yi kama da abin karɓa | Rata da aka tanada ya yi ƙanƙanta | Daidaita hangen nesa da ainihin rata a haɗin |
| Tsagewar jiki da ke bin canjin saiti maimakon canjin aiki | Ribbon da aka yi a kan mataki | Daidaiton cell da busbar a bussing |
| Lahani ɗaya a kan laminators da yawa yayin da injin bussing ɗaya ya tsaya cik | Zoben solder | Taimako a ƙarƙashin ribbon, sannan bayanin rufin ribbon |

Layi na uku shine wanda ya cancanci a riƙe a zuciya. Lokacin da lahani ya biyo sashin layin da bai canza ba, sashin da bai canza ba na iya zama sanadin, ba sarrafawa ba.

## Abin da za a riƙe a tashar bussing

Babu ɗaya daga cikin dalilai uku da za a iya bincika bayan lamination. Dole ne a riƙe su a tashar da ke yin haɗin, kuma a kan [na'urar haɗa igiya](https://www.ooitech.com/automatic-bussing-machine-dh200-y-solar-panel-busbar-soldering-equipment-ooitech.html) wannan yana nufin abubuwa huɗu:

- **Sanya.** Ya kamata a auna tazarar tsakanin gefen tantanin halitta da busbar kuma a zana shi, ba a ɗauka daga shirin ba. Matsalolin hangen nesa da jujjuyawar tsawon igiya duk suna motsa shi.
- **Daidaiton saman.** Bambancin tsayi tsakanin tantanin halitta da busbar a lokacin solder shine abin da ke ƙayyade tsawon ribbon. Kayan aikin tallafi da daidaiton kayan aiki suna yanke shawara.
- **Bayanin ribbon.** Kaurin rufi da daidaitonsa, ana duba su akan kayan da ke shigowa maimakon karanta su daga takardar bayanai. [Tsarin ribbon](https://www.ooitech.com/pv-ribbon-structure-and-types-flat-round-and-shaped.html) da kuma rufin sa suna ƙayyade nawa solder zai shiga cikin haɗin.
- **Lokacin dubawa.** Electroluminescence bayan lamination shine inda waɗannan lahani suke bayyana. Idan [dubawar EL](https://www.ooitech.com/el-testing-for-solar-panels-inline-vs-offline-setup.html) tana gudana a baya a cikin tsari, za a rasa tsagewar a lokacin da har yanzu ana iya gano ta zuwa tasha.

Bangaren lamination ma yana da muhimmanci, amma galibi a matsayin mai ƙarawa. Latsa wanda ke daidaita haɗin gwiwa daidai, tare da matakan vacuum da hawan matsin lamba suna yin abin da ya kamata su yi, yana kula da kowane haɗin gwiwa iri ɗaya. [Zagayen lamination](https://www.ooitech.com/solar-panel-production-process-lamination.html) shine inda geometry da aka gina a bussing a ƙarshe ya haɗu da sakamakonsa.

## Tambayoyin da ake yawan yi

### Me yasa tsagewar ke bayyana kawai bayan lamination?

Domin nauyin da ke karya gefen ana amfani da shi a cikin latsa. Haɗin gwiwa da kansa yana kama da na al'ada lokacin da aka yi shi; ribbon ɗin da ya wuce bai riga ya lanƙwasa ba, kuma zoben solder bai riga ya shiga matsin lamba ba. Lalacewar da ta riga ta kasance a cikin wafer kuma na iya kasancewa a rufe har sai matsin lamination ya buɗe ta ya zama tsagewar da za a iya karantawa a EL.

### Me yasa ake kiransa tsagewar rami na tsakiya?

Sunan ya fito daga inda ake ganin lahani a kan kammalallen module. Asalin inji shi ne haɗin tantanin halitta zuwa busbar, wanda shi ya sa dalilai uku da ke wannan shafi duk suna komawa zuwa matakin bussing maimakon ramin kansa.

### Shin matsalar ribbon ce ko matsalar soldering?

Matsalar geometry ce da ke bayyana ta hanyar haɗin soldered. Dalilai na ɗaya da na biyu kusan ba su da alaƙa da ribbon a matsayin samfur: rata da bambancin tsayi halaye ne na yadda ake sanya da tallafa sassan. Dalili na uku shi ne keɓanta, kuma a nan murfin ribbon ɗin yana da hannu kai tsaye.

### Shin ribbon mai kauri zai taimaka?

Zai ɗaga matakin da ribbon ɗin zai tsallaka a busbar, kuma zai sanya ƙarin abu a cikin duk wani zobe da ya samu. Hanyar da ke taimakawa gefen ita ce akasin haka: ƙaramin mataki da aka fi sarrafawa, rata da aka riƙe cikin taga ta, da murfi da ke yin ɗabi'a ɗaya a duk tsawon nadi.

### Shin za a iya kama wani abu daga cikin waɗannan kafin lamination?

Biyu daga cikin ukun za su iya, kuma ta hanyar auna kawai. Ratawar da aka tanada wani ma'auni ne da za ka iya dubawa a mahadar. Daidaito a bussing wani ma'auni ne da za ka iya dubawa a kan kayan aiki. Ana iya ganin zoben solder a mahadar idan wani ya neme shi, wanda shine dalilin da ya sa ya cancanci samun matakin dubawa bayan bussing da kuma bayan lamination.

### Shin wannan ya shafi modules marasa busbar?

Tsarin yana canzawa tare da mahadar. A kan [0BB module](https://www.ooitech.com/0bb-cell-technology-what-removing-the-busbar-changes.html) ribbon ɗin yana haɗe kai tsaye zuwa ƙananan yatsu, don haka babu gefen busbar da za a tsallaka kuma nauyin mahadar an rarraba shi a kan ƙari da yawa, ƙananan haɗi. Mahadar busbar da aka kwatanta a nan ita ce wacce tsayayyen tsiri mai kauri ya tsallaka gefen wafer na bakin ciki.

## Tunani na ƙarshe

Labarai uku daban-daban suna ƙarewa a cikin layi ɗaya mai duhu a cikin EL, kuma dalilin da ya sa suka cancanci rabuwa shi ne cewa suna buƙatar gyare-gyare uku daban-daban. Ratawar matsalar sanyawa ce. Matakin matsalar daidaito ce. Zoben matsalar kayan aiki da tallafi ce. Layin da ke ɗaukar duk ukun a matsayin "matsalar lamination" zai kashe lokacinsa wajen daidaita matsi wanda ba shi ne sanadin ba.

Abin da ya zama gama gari shi ne cewa tsiri na ribbon da ke ƙarƙashin tashin hankali hanya ce ta ɗaukar nauyi, kuma gefen wafer shi ne mafi ƙunci a kanta. Ƙananan sel sun sa wannan gefen ya fi ƙunci, kuma taga aiki da ta kasance tana ɗaukar kashi goma na millimita na rashin daidaituwa ba ta ƙara yin hakan ba.

**Karatun da ke da alaƙa:** [Abin da ribbon na PV ke yi: ayyuka uku, musanya ɗaya](https://www.ooitech.com/what-a-pv-ribbon-does-three-jobs-one-trade-off.html) · [Kayan ribbon na PV: ainihin tagulla, tauri da shafi](https://www.ooitech.com/pv-ribbon-materials-copper-core-hardness-and-coating.html) · [Tsarin ribbon na PV da nau'ikansa: lebur, zagaye da siffa](https://www.ooitech.com/pv-ribbon-structure-and-types-flat-round-and-shaped.html) · [Injin bussing ta atomatik na DH200-Y](https://www.ooitech.com/automatic-bussing-machine-dh200-y-solar-panel-busbar-soldering-equipment-ooitech.html) · [Injin bussing na rabin-cell na HDX200-P](https://www.ooitech.com/hdx200-p-half-cell-auto-bussing-machine-automatic-busbar-welding-machine-for-solar-panel-production.html) · [Injin layup da bussing na SAW-100A](https://www.ooitech.com/automatic-layup-and-bussing-integrated-machine-saw-100a-solar-panel-production-equipment-ooitech.html) · [Laminator na panel ɗin rana: an bayyana tsarin lamination](https://www.ooitech.com/solar-panel-production-process-lamination.html) · [Yadda za a zaɓi laminator na module ɗin rana da ya dace](https://www.ooitech.com/how-to-choose-the-right-solar-module-laminator.html) · [Gwaje-gwajen amincin module na PV: musabbabin gazawar cell da module](https://www.ooitech.com/pv-module-reliability-tests-list-cell-vs-module-failure-causes.html) · [Injin tabber da stringer: yadda yake aiki, yadda za a zaɓe shi](https://www.ooitech.com/tabber-and-stringer-machine-how-it-works-how-to-choose.html)

Adadin kauri na wafer da busbar na tsakiya su ne ƙimar da aka saba ambata a cikin tushen bayanan kuma sun bambanta bisa ga mai bayarwa da ƙira. Maganganu game da sassan tashin hankali na ribbon F1 da F2 suna bayyana alkiblar nauyin da ke wurin haɗin; rabon da ke tsakaninsu ya biyo baya daga kusurwar ribbon kuma ba ƙimar da aka auna ba ce.

Masu alaƙa: [Wurare masu zafi, tsage-tsage da PID: gazawar module guda uku a hankali](https://www.ooitech.com/hot-spots-microcracks-and-pid-three-slow-module-failures.html) yana sanya wannan lahani na haɗin gwiwa cikin babban hoto na asarar module a hankali.

Masu alaƙa: [Hanyoyin haɗa ƙwayoyin hasken rana: jagora ta kowane yanki](https://www.ooitech.com/solar-cell-stringer-mechanisms-a-zone-by-zone-guide.html). Haɗin bussing ɗin yana gazawa a ƙasa da stringer, akan haɗin da stringer ya yi.

## Ƙarin karatu da bayanan baya

Kayan tunani na jama'a kan wannan batu, wanda ƙungiyoyin da ke kula da taswirar fasahar masana'antar da bayanan kasuwa suka wallafa:

- [VDMA — Taswirar Fasahar Ƙasa da Ƙasa don Photovoltaic (ITRPV)](https://www.vdma.org/international-technology-roadmap-photovoltaic)
- [pv mujallar — labaran masana'antar PV na duniya da ɗaukar fasaha](https://www.pv-magazine.com/)
- [Fraunhofer ISE — Rahoton Photovoltaics](https://www.ise.fraunhofer.de/en/publications/studies/photovoltaics-report.html)

---

##### Tags :

![](/template/ooitech/assets/img/shape/06.png)

![](https://cdn.ooitech.com/runtime/image/w800_h700_fitblur_v2_w800_h700_fitblur_v2_1757399770541443.webp)

### Nemi Farashi

Duk abubuwan da aka ɗora suna da tsaro kuma sirri ne.

## Muna isar da gwanintar da za ka iya amincewa sabis ɗinmu

Kayan aiki kai tsaye daga masana'anta.

![](/template/ooitech/assets/img/icon/money-2.svg)

### Fa'idodin Rage Kuɗi

Muna ba da ƙima ta musamman, muna haɓaka sakamako yayin da muke rage kasafin kuɗi ga abokan ciniki.

![](/template/ooitech/assets/img/icon/staff.svg)

### Ƙungiyar Ƙwarewarmu

Kwararrun ma'aikatanmu sun ƙware a sababbin hanyoyin magance matsaloli da dabarun da aka keɓance.

![](/template/ooitech/assets/img/icon/certified.svg)

### Fiye da Shekaru 15 na Ƙwarewar Masana'antu

Ƙwarewa mai zurfi tana tabbatar da sakamako masu dogaro, masu bin zamani, da tabbatattu don nasara.

![](https://cdn.ooitech.com/static/upload/image/20250910/1757477357667605.webp )

![](https://cdn.ooitech.com/static/upload/image/20250910/1757477724911512.webp)

![](/template/ooitech/assets/img/shape/06.png)

## Abin da Abokin Cinikinmu Ya ce game da mu

Shaidun abokan ciniki sun yaba da zurfin fahimtarmu game da ƙalubalen su, wanda ke haifar da sababbin hanyoyin magance matsaloli da riba mai ƙarfi. Haɗin gwiwa na dogon lokaci—wasu fiye da shekaru goma—suna nuna amincewarsu da gamsuwa. Labaran nasarar su suna motsa mu don ci gaba da wuce tsammanin su. [Ƙara Sani **](#quote-form)

![](/template/ooitech/assets/img/icon/quote.svg)

Godiya ga Ooitech don samar da kayan aikin samarwa na atomatik cikakke—shigar da ku da sabis na bayan siyarwa sun yi kyau sosai.

![](https://cdn.ooitech.com/runtime/image/w800_h600_fitblur_v2_2026041720921238.webp)

### Amjad

![](/template/ooitech/assets/img/icon/quote.svg)

na gode da goyon bayan ƙwararrun ooitech da sabis na bayan lokaci.

![](https://cdn.ooitech.com/runtime/image/w800_h600_fitblur_v2_1784509010217979.webp)

### Diarra Daga Afirka

![](/template/ooitech/assets/img/icon/quote.svg)

Mutum mai babban rai. Na gode sosai da ziyarar ku Mista Wu. Na gode sosai da ayyukan da aka bayar wajen shigar da kayan aiki da horar da dalibai na. Mutum mafi kirki kuma ƙwararre a fanninsa.

![](https://cdn.ooitech.com/runtime/image/w800_h600_fitblur_v2_2026041716444445.webp)

### Jizzakh Polytechnic Institute

![](/template/ooitech/assets/img/icon/quote.svg)

Godiya ga Ooitech don samar da kayan aikin gwajin ƙwayar hasken rana na BC da suka dace sosai.

![](https://cdn.ooitech.com/runtime/image/w800_h600_fitblur_v2_1776426122864564.webp)

### KTECH

![](/template/ooitech/assets/img/icon/quote.svg)

Na sake godewa sosai don babban taimako na inganta da gyara masana'anta da kuma koya wa ma'aikata yadda ake amfani da injinan

![](https://cdn.ooitech.com/runtime/image/w800_h600_fitblur_v2_1757479675272137.webp)

### Mark

BIPV Philippines

## Sabbin Kayayyakin Mu

![SS-2500B Tabber da Stringer: 2400 Cells/h, 3-20BB](https://cdn.ooitech.com/runtime/image/w800_h600_fitblur_v2_1774258018905303.webp)

- [** ooitech](./SS-2500B-Full-Automatic-Solar-Cell-Tabber-Stringer-Machine-High-Speed-Production-Line-Equipment.html)
- [** 37053](./SS-2500B-Full-Automatic-Solar-Cell-Tabber-Stringer-Machine-High-Speed-Production-Line-Equipment.html)

### SS-2500B Tabber da Stringer: 2400 Cells/h, 3-20BB

SS-2500B cikakken atomatik tabber stringer inji don crystalline silicon solar cells tare da 2400PCS/H iya aiki, yana da infrared soldering

![Injin Liƙa Tef Ta Atomatik: Zagayowar 25s, ±2mm](https://cdn.ooitech.com/runtime/image/w800_h600_fitblur_v2_1774350079476146.webp)

- [** Rachael](./automatic-tape-sticking-machine-for-solar-panel-production-line-ooitech.html)
- [** 81810](./automatic-tape-sticking-machine-for-solar-panel-production-line-ooitech.html)

### Injin Liƙa Tef Ta Atomatik: Zagayowar 25s, ±2mm

Injin Liƙa Tef ɗin Ooitech ta atomatik yana liƙa tef ɗin manne a kan igiyoyin ƙwayoyin rana da daidaito da sauri.

![Haɗin String: Jagorar Ribbon Busbar na Rana](https://cdn.ooitech.com/runtime/image/w800_h600_fitblur_v2_2026032713037538.jpg.webp)

- [** Rachael](./Interconnection-Busbar-for-Solar-Module-Assembly-High-Performance-Current-Collection-Solution.html)
- [** 96974](./Interconnection-Busbar-for-Solar-Module-Assembly-High-Performance-Current-Collection-Solution.html)

### Haɗin String: Jagorar Ribbon Busbar na Rana

Ingantattun hanyoyin busbar na haɗin kai don haɗa kayan aikin rana, mai ɗauke da gini na tagulla mai tsafta da aka yi da tin

![Na'urar Laminator BIPV Mai Dakuna Biyu Mai Layer Daya](https://cdn.ooitech.com/runtime/image/w800_h600_fitblur_v2_1774438506273987.webp)

- [** Rachael](./single-layer-double-chamber-automatic-bipv-laminator-otcy-2754dd-ooitech-solar-panel-lamination-equipment.html)
- [** 63368](./single-layer-double-chamber-automatic-bipv-laminator-otcy-2754dd-ooitech-solar-panel-lamination-equipment.html)

### Na'urar Laminator BIPV Mai Dakuna Biyu Mai Layer Daya

Ooitech OTCY-2754DD Single Layer Double Chamber Automatic BIPV Laminator yana da wuraren lamination guda biyu na 2700x5400mm, dumama biyu na sama da ƙasa

![Mai rufe Panel Solar da Tef: Silicone, Butyl, PET](https://cdn.ooitech.com/runtime/image/w800_h600_fitblur_v2_2026032711586064.jpg.webp)

- [** Rachael](./PV-Module-Sealant-Tape-Solutions-Essential-Components-for-Solar-Panel-Reliability.html)
- [** 73265](./PV-Module-Sealant-Tape-Solutions-Essential-Components-for-Solar-Panel-Reliability.html)

### Mai rufe Panel Solar da Tef: Silicone, Butyl, PET

Mai rufe hasken rana da tef don haɗa module: silicone mai rufe firam, tef na butyl da tef na rufin busbar, mai jure UV don fallasa waje na shekaru 25.

![SC-20D Na'urar Yankan Ƙwayoyin Hasken Rana mai Laser Biyu](https://cdn.ooitech.com/runtime/image/w800_h600_fitblur_v2_1773917787610971.webp)

- [** ooitech](./SC-20D-Full-Automatic-Solar-Cell-Laser-Cutting-Machine-High-Precision-Wafer-Scribing-Equipment.html)
- [** 51321](./SC-20D-Full-Automatic-Solar-Cell-Laser-Cutting-Machine-High-Precision-Wafer-Scribing-Equipment.html)

### SC-20D Na'urar Yankan Ƙwayoyin Hasken Rana mai Laser Biyu

SC-20D ita ce sigar ci gaba ta SC-20A, wadda aka ƙera ta musamman don samar da ƙwayoyin hasken rana na shingled, mai kawunan laser biyu da lasers biyu suna aiki